欢迎访问《人工晶体学报》官方网站,今天是 分享到:

人工晶体学报 ›› 2021, Vol. 50 ›› Issue (5): 920-926.

• 研究论文 • 上一篇    下一篇

微波加热制备含稀土(La2O3)矿渣微晶玻璃研究

赵广凯1, 徐文策1, 刘赛余1,2, 张宇轩1,3, 吴楠楠2, 刘芳1, 欧阳顺利1   

  1. 1.内蒙古科技大学,白云鄂博矿多金属资源综合利用重点实验室,包头 014010;
    2.内蒙古科技大学理学院,包头 014010;
    3.内蒙古科技大学材料与冶金学院,包头 014010
  • 收稿日期:2020-12-16 出版日期:2021-05-15 发布日期:2021-06-15
  • 通讯作者: 欧阳顺利,博士,教授。E-mail:ouyangshunli@imust.cn
  • 作者简介:赵广凯(1995—),男,黑龙江省人,硕士研究生。E-mail:2246562732@qq.com
  • 基金资助:
    国家自然科学基金(11964025,11564031);内蒙古自治区重大基础研究开放课题(0406091701);内蒙古科技大学创新基金项目-优秀青年科学基金(2019YQL06);内蒙古自治区自然科学基金(2018LH02004);内蒙古科技创新引导项目

Preparation of La2O3 Slag Glass-Ceramics by Microwave Heating

ZHAO Guangkai1, XU Wence1, LIU Saiyu1, 2, ZHANG Yuxuan1,3, WU Nannan2, LIU Fang1, OUYANG Shunli1   

  1. 1. Key Laboratory of Integrated Exploitation of Bayan Obo Multi-Metal Resources, Inner Mongolia University of Science and Technology, Baotou 014010, China;
    2. School of Science, Inner Mongolia University of Science and Technology, Baotou 014010, China;
    3. Materials and Metallurgy School, Inner Mongolia University of Science and Technology, Baotou 014010, China
  • Received:2020-12-16 Online:2021-05-15 Published:2021-06-15

摘要: 利用矿渣制备微晶玻璃是提高矿产资源利用率的主要形式之一。本文以白云鄂博尾矿为原料,采用微波一步法制备了CaO-MgO-Al2O3-SiO2(CMAS)系辉石相矿渣微晶玻璃。选择835 ℃作为晶化温度,研究了微波加热对微晶玻璃析晶行为和微观组织的影响。以La2O3作为研究变量探讨了La2O3添加对矿渣微晶玻璃析晶行为的作用。与传统的热处理制度相比,微波加热可以在较短的时间内达到较高的析晶效果。同时La2O3的添加促进了晶粒细化。由拉曼光谱分析,La离子添加会导致玻璃网络中桥氧的增多,促进了辉石相析晶。在La的添加量为4%(质量分数)时硬度最高,达到了829.22 MPa。

关键词: 白云鄂博尾矿, 微波法, 矿渣微晶玻璃, 氧化镧, 拉曼光谱

Abstract: Using slag to prepare slag glass-ceramics is one of the main ways to improve the utilization rate of mineral resources. CaO-MgO-Al2O3-SiO2(CMAS) series pyroxene phase slag glass-ceramics were prepared using Bayan Obo tailings as raw materials by microwave one-step method. 835 ℃ was choosed as the crystallization temperature and the influence of microwave heating on the crystallization behavior and microstructure of glass-ceramics were studied. Effect of La2O3 addition on the crystallization behavior of slag glass-ceramics were discussed using La2O3 as the research variable. Compared with traditional heat treatment system, the microwave heating achieves higher crystallization effect in a shorter time. Here, the addition of La2O3 promotes grain refinement. According to the analysis of Raman spectroscopy, the addition of La ion will cause the increase of bridging oxygen in the glass network and increase the tightness and integrity of the crystal. The hardness is the highest when the addition of La is 4% (mass fraction), and the Vickers hardness reaches 829.22 MPa.

Key words: Bayan Obo tailing, microwave method, slag glass-ceramics, La2O3, Raman spectroscopy

中图分类号: